Laser Welding Defects: Causes and Prevention

Laser welding produces a specific set of defects that differ from arc welding defects in both cause and appearance. Understanding the defect-cause relationship in laser welding is the prerequisite for effective troubleshooting — adjusting parameters at random rarely resolves a defect systematically, and some laser welding defects have counterintuitive causes (the fix is to increase speed, not reduce it; to increase power, not reduce it).

This article is the comprehensive defect reference for laser welding — covering all major defect types, organized by defect appearance so that the diagnostic path starts with what you see.


Defect 1: Porosity

Spherical porosity (rounded pores, random distribution)

Laser Welding Defects

Appearance: Round pores visible in cross-section or on X-ray; may appear as surface pitting if pores are near the surface.

Root causes:

  • Hydrogen from surface contamination: Oil, fingerprints, cutting fluid residue, or moisture on the base metal or filler wire. Hydrogen dissolves in liquid metal and is expelled as bubbles during solidification. This is the most common porosity cause in stainless and aluminum welding.
  • Moisture in shielding gas: Water vapor contamination of argon or helium shielding gas. Check gas purity and hose connections for moisture ingress.
  • Shielding gas inadequate: Atmospheric oxygen or nitrogen entrainment in the weld pool. Increase flow rate, improve nozzle position, eliminate air drafts.
  • Zinc or cadmium from coatings: Coating vaporization (galvanized steel, cadmium-plated parts) generates vapor that becomes porosity if it cannot escape the pool.

Prevention: Clean with acetone immediately before welding. Verify shielding gas purity and hose integrity. Apply the gap technique for coated materials.

Elongated porosity (wormhole / piping porosity)

Causes-and-Solutions-of-Pores-in-Laser-Welding

Appearance: Elongated pores aligned with the weld direction; sometimes open at the root surface. Distinct from spherical porosity by shape and orientation.

Root causes:

  • Keyhole instability: The keyhole collapses and re-establishes erratically during welding. When the keyhole collapses, the gas inside cannot escape before solidification and is trapped as an elongated pore along the collapse zone. This is the laser-welding-specific porosity mechanism — it does not occur in arc welding.
  • Keyhole instability is caused by: power too low for the travel speed (the keyhole cannot sustain itself), excessive travel speed, or focus position creating a power density at the edge of the keyhole threshold.

Prevention: Increase power by 5–10% to stabilize the keyhole, or reduce speed by 10%. Verify focus position is not creating a power density at the conduction-keyhole boundary. Pulsed or wobble welding modes can stabilize keyhole dynamics.

Centerline porosity (pores along the weld centerline, visible in cross-section)

Why-do-Pores-Occur-during-Laser-Welding

Appearance: Chain of small pores along the weld centerline, visible in longitudinal section.

Root causes: Solidification pattern directing the last liquid to solidify at the centerline, where dissolved gas is rejected and concentrated. Common in aluminum alloys and in welds with a high depth-to-width ratio (keyhole welds at high power, slow speed).

Prevention: Adjust the weld pool width-to-depth ratio by defocusing slightly (increase spot size) or by using wobble welding to widen the pool. Using ER4043 filler (for aluminum) improves the solidification behavior and reduces centerline porosity tendency.


Defect 2: Solidification Cracking (Hot Cracking)

Cracks-Formation-Over-Aluminum-Surfacese

Appearance: Cracks along the weld centerline, typically following the weld direction. May be open at the surface or sub-surface (visible only in cross-section).

Root causes:

  • Wide freezing range alloy without filler: 6061 aluminum and similar alloys have a wide liquidus-solidus temperature interval. The last liquid at the centerline cannot accommodate the tensile strain from cooling — the solid metal contracts while the centerline is still liquid, and the liquid tears apart. The laser welding aluminum article covers this mechanism in detail.
  • Highly restrained joint: High restraint (rigid fixturing, large assembly) increases the tensile stress acting on the solidifying weld centerline.
  • High dilution of crack-susceptible base metal into the weld pool: If the base metal is crack-susceptible and the filler is insufficient to change the effective composition.

Prevention: Use filler wire for crack-susceptible alloys (ER4043 or ER5356 for 6061 aluminum). Reduce joint restraint where possible. Reduce travel speed to widen the weld pool and change the solidification front angle.

Do not confuse with: Liquation cracking — cracks in the partially melted zone adjacent to the weld, not at the centerline. Liquation cracking in the HAZ results from low-melting grain boundary phases becoming liquid during welding and cracking under stress.


Defect 3: Underfill and Undercut

Underfill

the weld is recessed rather than flush or convex.

Appearance: The weld bead cross-section is below the level of the base metal surface — the weld is recessed rather than flush or convex.

Root causes:

  • Autogenous welding at high speed on material with significant gap: The weld pool volume is insufficient to fill the joint at high speed. The metal melted from both sides cannot fill a gap and maintain flush level simultaneously.
  • Insufficient filler wire speed: If filler wire is used and the feed rate is too low for the joint gap or the welding speed, the bead will underfill.

Prevention: Reduce travel speed to allow the pool to fill the joint, or increase filler wire feed rate. For persistent underfill, close the joint gap in the fixturing.

Undercut

Appearance: A groove alongside the weld bead, recessed below the base metal surface. The undercut reduces the effective cross-section at the weld toe.

Root causes:

  • Travel speed too high for the power level: The pool is narrow and hot at the edges, and the metal at the weld edge melts and flows into the pool without being replaced — leaving a groove.
  • Power too high at the weld edge: For fillet welds, excessive power deposits energy at the weld toe, melting the base metal without adding enough fill to compensate.

Prevention: Reduce travel speed by 10–15%. For fillet welds, check filler wire placement and adjust beam position slightly toward the weld pool center.


Defect 4: Lack of Fusion

Sidewall lack of fusion

Appearance: Unfused zone between the weld bead and one or both of the base metal faces at the sidewall. Visible in cross-section; may be detected by ultrasonic testing before cross-section.

Root causes:

  • Beam offset from joint centerline: If the laser beam is not centered on the joint, one sidewall receives more energy than the other. The less-heated side may not reach fusion temperature, leaving an unbonded interface.
  • Power too low for the travel speed: Insufficient power density to melt both sidewalls simultaneously at the travel speed used.

Prevention: Verify beam position relative to joint center (tape test or burn mark on tape). Reduce travel speed or increase power.

Root lack of fusion (incomplete penetration)

Appearance: The weld does not penetrate the full material thickness — visible as a “notch” at the root in cross-section.

Root causes: Power insufficient for material thickness at the travel speed used. Joint gap exceeding the weld pool’s bridging capability. Focus position too positive (beam above surface) — reduced power density at depth.

Prevention: Increase power, reduce speed, or shift focus negative. Verify gap tolerance is within specification.


Defect 5: Burn-Through

Burn-Through laser welding

Appearance: Hole or chain of craters through the weld, especially on thin material.

Root causes and prevention: Covered comprehensively in the laser welding thin metal article. The primary cause on thin material (under 1.5 mm) is travel speed too slow, not power too high. The fix is to increase travel speed and accept slightly reduced penetration, then increase power to compensate.


Defect 6: Spatter

Appearance: Metallic particles scattered around the weld zone; may adhere to the base metal surface or be ejected to surrounding areas.

Root causes:

  • Keyhole instability: The most common cause of high spatter in laser welding. Keyhole collapse events eject molten metal from the pool — the same mechanism that causes elongated porosity also causes spatter when the ejected metal exits the pool rather than being re-absorbed.
  • Contamination: Oil, oxide, or coating burns explosively in the keyhole, creating pressure spikes that eject spatter.
  • Excessive power density: Very high power density (especially at small spot size) drives violent vapor pressure that ejects pool metal. Reducing power or defocusing reduces spatter.

Prevention: Address keyhole instability (see elongated porosity above). Clean the surface. For inherently high-spatter materials (galvanized steel, copper, brass), use wobble welding or pulsed mode to reduce peak vapor pressure.


Defect 7: Distortion

Appearance: Angular deformation (rotation around the weld line), transverse shrinkage (joint gap narrowing), or longitudinal bowing after welding.

Root causes and prevention: Covered in detail in the laser welding HAZ article. The short summary: all three distortion types reduce with lower heat input — faster travel speed is the primary lever. For thin stainless, rigid fixturing through the full thermal cycle is the most reliable distortion control.


Defect 8: Humping

Appearance: Periodic bulges along the weld bead, spaced at regular intervals. The bead is not smooth — it alternates between swellings and narrower sections. This is a high-speed welding defect.

Root causes: Humping is a hydrodynamic instability that develops at high travel speeds when the weld pool becomes elongated beyond a critical aspect ratio. The elongated pool breaks into discrete pools that then solidify into humps. This occurs specifically when travel speed exceeds a material-dependent threshold — typically above 4–8 m/min on stainless and above 3–5 m/min on aluminum.

Prevention: Reduce travel speed below the humping threshold. Alternatively, use a beam oscillation (wobble) to widen the weld pool, which raises the humping threshold speed. Defocusing to increase the beam spot size also raises the humping threshold.


Defect 9: Heat Tinting and Oxidation

Discoloration around the weld zone

Appearance: Discoloration around the weld zone (gold, blue, purple, gray — in order of increasing temperature). On stainless, indicates oxidation that has degraded the passive layer and corrosion resistance.

Root causes:

  • Inadequate shielding gas flow: The weld face is not protected from atmospheric oxygen during and after welding.
  • Air drafts disrupting the shielding gas: Shop ventilation, open doors, or fans near the welding station.
  • Root oxidation: The weld root (back surface) is not shielded. Requires backing gas purge for full-penetration stainless welds.

Prevention: Verify shielding gas flow rate (minimum 12 L/min for standard argon shielding), verify nozzle position and aim, shield the work area from air movement, and add backing gas purge for critical stainless applications. See the laser welding shielding gas article for full gas selection guidance.


Defect 10: Lack of Penetration at Weld Start

Appearance: The first 5–20 mm of the weld is narrow, shallow, or has surface roughness not present along the rest of the weld length.

Root causes:

  • Pierce residue: The pierce point deposits molten material that the weld traverses, creating an inconsistent starting condition.
  • Thermal lag: At weld initiation, the material is cold and absorbs laser energy less efficiently until the keyhole establishes. The weld pool transitions from conduction-mode to keyhole during the first few millimetres.

Prevention: Use a lead-in (start the weld in the waste material and run into the joint boundary). Use a power ramp (start at reduced power for 20–50 ms to initiate the keyhole before full power). Pierce in the waste area offset from the joint boundary.


Defect Diagnostic Quick Reference

Observed defect First check Second check Likely fix
Spherical porosity Surface cleanliness Shielding gas purity Clean with acetone; verify gas
Elongated/wormhole porosity Power level for speed Focus position Increase power 5–10%
Centerline cracking Filler wire present? Alloy type Add/increase filler wire
Underfill Gap size Filler speed Reduce gap; increase wire feed
Undercut Travel speed Power level Reduce speed 10%
Burn-through Travel speed (thin material) Power level Increase speed first
Spatter Surface contamination Power density Clean surface; reduce power or wobble
Humping Travel speed Spot size Reduce speed; increase spot size
Heat tinting Gas flow rate Air drafts Increase flow; shield area
Start-of-weld defect Lead-in used? Pierce location Add lead-in; offset pierce to waste

Frequently Asked Questions

How do I tell the difference between hydrogen porosity and keyhole instability porosity?

Hydrogen (contamination) porosity produces spherical pores randomly distributed through the weld cross-section. Keyhole instability produces elongated pores (worm holes) aligned with the weld direction, typically at or near the weld centerline. The distinction is visible in cross-section and X-ray: round random = clean the surface; elongated aligned = adjust power or speed to stabilize the keyhole.

Why does my laser weld spatter when I increase power?

Counterintuitively, increasing power above the minimum needed for penetration at a given travel speed increases spatter. The excess power creates a more energetic keyhole with higher vapor pressure — which ejects more melt from the pool as spatter. The correct response to excess spatter from a stable keyhole is to reduce power to the minimum that achieves penetration, or to increase travel speed proportionally. Spatter from keyhole instability (where the keyhole is collapsing and re-establishing) requires increasing power, not reducing it — the two causes produce identical visual spatter but require opposite fixes.

Does weld start porosity indicate a contamination problem?

Not necessarily. Weld start defects (narrow, shallow first section; start-of-weld porosity) are often caused by the thermal lag during keyhole formation rather than surface contamination. Run the defect in question: if porosity appears throughout the weld length, contamination is the likely cause. If porosity is confined to the first 5–10 mm of the weld and the remainder is clean, thermal lag or pierce residue is the cause. Use a lead-in or power ramp to address it.


References

  1. AWS C7.2M/C7.2, Recommended Practices for Laser Beam Welding, Cutting, and Drilling, AWS, Miami, FL, current edition. (Laser weld defect classification; inspection methods; process parameters affecting defect formation — the primary process standard for the defect analysis in this article.)
  2. ASM Handbook, Volume 6: Welding, Brazing, and Soldering, 10th Edition. ASM International, 1993. (Porosity mechanisms; solidification cracking; lack of fusion causes; undercut and underfill — the materials science reference for the defect mechanisms described.)
  3. Duley, W.W., Laser Welding. Wiley-Interscience, New York, 1999. (Keyhole instability and elongated porosity; humping formation mechanism; spatter generation — the dedicated laser welding reference for the laser-specific defect mechanisms in this article.)
  4. ARCUSCNC, Laser Welding Machine Operation Manual, ARCUSCNC, 2024. (Machine-specific parameter configuration for keyhole stabilization; wobble and pulsed mode settings for spatter reduction — the machine reference for the parameter recommendations in this article.)
Dr. Liu Che

Leave A Comment

No products in the cart.