Laser Welding Galvanized Steel Without Excess Porosity

Galvanized steel presents a specific welding problem that has nothing to do with the steel itself: the zinc coating boils at 907°C, while steel melts at approximately 1,500°C. By the time the laser has heated the steel substrate to its melting point, the zinc coating has already vaporized — and that zinc vapor, generated directly beneath and within the molten weld pool, has nowhere to go except through the liquid steel above it. The result, without specific process adjustments, is severe porosity from trapped zinc vapor bubbles.

This is a fundamentally different porosity mechanism from the hydrogen porosity that affects aluminum welding or the gas shielding porosity that affects stainless. Understanding the zinc vapor mechanism is what makes the solution — controlled venting, not just “more shielding gas” — make sense.


Why Galvanized Steel Porosity Is a Vapor Pressure Problem, Not a Contamination Problem

Laser Welding Galvanized Steel

When the laser beam heats galvanized steel, the sequence of events is:

  1. The zinc coating (typically 7–25 μm thick, depending on coating class) reaches its boiling point (907°C) before the underlying steel reaches its melting point (~1,500°C)
  2. Zinc vaporizes at the steel-zinc interface, both at the surface where the beam is incident and — critically — at the joint interface in a lap joint, where zinc coating exists on both mating surfaces
  3. The zinc vapor, generated at a location now beneath molten or about-to-melt steel, must escape through the weld pool to reach the atmosphere
  4. If the vapor cannot escape fast enough relative to the weld pool’s solidification rate, it becomes trapped as porosity

This is a pressure and timing problem: the zinc vapor needs an escape path, and it needs that path to exist for long enough (i.e., the weld pool needs to stay liquid long enough) for the vapor to clear before solidification traps it.

Why this is worse on lap joints than butt joints: In a butt joint, the zinc coating burns off the top surface before reaching the joint, and the vapor has direct access to the atmosphere above the weld pool. In a lap joint (the configuration used in the majority of galvanized sheet metal fabrication — automotive body panels, HVAC ductwork, appliance enclosures), the zinc-coated faying surfaces are sandwiched together, and any zinc vapor generated at that interface must travel sideways through the joint and then up through the weld pool — a much longer and more obstructed escape path.


The Gap Technique: The Primary Solution for Lap Joints

Hot-dipped-galvanized-steel-no-preparation

The most widely used and most effective solution for galvanized lap joint welding is to introduce a deliberate, controlled gap between the two sheets at the joint — typically 0.1–0.3 mm, depending on material thickness and zinc coating weight.

Why the gap works: The gap provides a physical escape channel for zinc vapor generated at the faying surface. Instead of being trapped between two tightly clamped sheets, the vapor can travel laterally through the gap and escape before the weld pool solidifies over it.

Methods for creating the gap:

Mechanical spacers: Small tabs or dimples formed into one of the two sheets at intervals along the joint (every 50–100 mm) create a controlled, repeatable gap without requiring precision shimming at every joint.

Laser-cut edge preparation: For sheets that will be laser cut and then laser welded (a common workflow), a slight relief can be designed into the laser cutting program at the joint edge — for example, a very slight scallop or step that creates the venting gap when the two cut edges are assembled.

Clamping force control: Reducing clamping force at the joint (rather than the high clamping pressure typically used for tight-fit-up laser welding) allows the natural surface waviness of the sheets to create micro-gaps sufficient for venting, particularly on thinner gauge material with inherent surface irregularity.

Gap size guidance by material thickness:

Material thickness Zinc coating (typical) Recommended gap
0.5–1.0 mm Z275 (20 μm) 0.05–0.10 mm
1.0–1.5 mm Z275 (20 μm) 0.10–0.15 mm
1.5–2.5 mm Z275–Z450 0.15–0.25 mm
2.5+ mm Z450+ (heavy coating) 0.20–0.30 mm

Heavier zinc coatings generate proportionally more vapor and require a larger gap. If the gap exceeds the joint’s gap tolerance for adequate fusion (covered in the laser cut stainless welding prep article for the general principle), filler wire becomes necessary to bridge the gap while still providing the venting function.


Parameter Adjustments to Manage Zinc Vapor

galvanneal-box-section-16ga-laser-welding

Beyond the joint gap, several process parameter adjustments reduce porosity risk on galvanized steel:

Reduced travel speed at the start of the weld

A slightly slower travel speed at weld initiation (the first 10–20 mm) allows more time for the initial zinc vaporization burst to clear before the weld pool stabilizes into steady-state. Many porosity defects in galvanized welding cluster at the weld start rather than distributing evenly along the joint length, because the initial zinc vapor volume is highest before a stable vent path has established.

Power modulation (pulsed or wobble mode)

Continuous wave (CW) welding at constant power maintains a continuously molten pool with limited opportunity for vapor to escape between pulses. Pulsed mode (power oscillating between a high peak and a lower base level) or wobble welding (the beam oscillates transversely while advancing) both create brief moments of reduced pool depth or increased pool surface area that improve vapor escape compared to steady CW welding at the same average power.

Wobble welding specifically: The transverse oscillation effectively widens the weld pool surface area relative to its volume, giving zinc vapor more surface area to escape through per unit of weld pool volume. Wobble amplitude of 0.3–0.8 mm at 50–200 Hz oscillation frequency is a typical starting point for galvanized steel; verify against the parameter window for your specific laser system.

Slightly reduced power, slightly slower speed

Counter to the general principle of minimizing heat input (which reduces distortion, per the laser welding HAZ article), galvanized steel welding sometimes benefits from a marginally longer weld pool dwell time — achieved by a modest power reduction combined with a proportional speed reduction to maintain the target heat input. The longer dwell time at moderate intensity (rather than a fast, intense weld) gives zinc vapor more time to escape before solidification, at the cost of a slightly wider HAZ than the absolute minimum achievable on the same material without zinc coating.


Pre-Weld Zinc Coating Removal: When It’s Worth It

Laser-lap-welding-galvannealed-steel

For the highest-quality galvanized welds (where porosity must be essentially eliminated, not just managed), removing the zinc coating from the joint area before welding eliminates the zinc vapor problem at its source.

Methods:

  • Mechanical grinding: Grinding a 5–10 mm strip on each side of the joint line removes the zinc coating from the weld and HAZ area. Effective but adds a manual operation and creates bare steel that requires post-weld corrosion protection at the stripped zone.
  • Laser zinc ablation (pre-weld pass): A lower-power laser pass immediately before the welding pass selectively vaporizes the zinc coating from the joint area without melting the steel substrate. This can be integrated into the same machine cycle as the weld itself, using a defocused or reduced-power pre-pass.
  • Chemical stripping: Acid or alkaline stripping solutions remove zinc coating from the joint area — practical for batch pre-processing but adds a wet chemical process step to an otherwise dry fabrication workflow.

When zinc removal is worth the added process step:

  • Critical structural welds where porosity-related strength reduction cannot be tolerated
  • Cosmetic welds where surface appearance must be free of porosity-related pitting
  • Hermetic seal applications where even minor porosity creates an unacceptable leak path

When the gap technique alone is sufficient:

  • General production fabrication (HVAC ductwork, appliance housings, automotive non-structural panels) where the gap technique combined with parameter optimization produces acceptable porosity levels for the application’s actual requirements
  • High-volume production where the added cost and cycle time of zinc removal is not justified by the application’s quality requirement

Post-Weld Corrosion Protection at the Weld Zone

Regardless of the porosity management approach, the weld zone and immediately surrounding HAZ lose the original zinc galvanic protection — the zinc coating in this area has been vaporized or removed during welding. This creates a localized corrosion vulnerability that must be addressed for any application where the welded assembly will see corrosive service.

Cold galvanizing compound (zinc-rich paint): Applied to the weld bead and HAZ after welding, zinc-rich paint (typically 65–95% zinc by weight in the dry film) restores galvanic protection to the affected zone. This is the standard field and shop repair method for galvanizing damage from any cause, including welding.

Zinc spray metallizing: For higher-performance applications, thermal spray zinc metallizing applied to the weld zone provides more durable protection than cold galvanizing compound, approaching the original hot-dip galvanizing performance.

Re-dipping (full assembly): For fabricated assemblies where the entire structure will be hot-dip galvanized after fabrication (rather than welding pre-galvanized components), this consideration does not apply — the galvanizing happens after all welding is complete, and the entire structure including weld zones receives full coating coverage.


Frequently Asked Questions

Why does galvanized steel produce more weld porosity than bare steel?

The zinc coating boils at 907°C while steel melts at approximately 1,500°C. Zinc vaporizes before the steel reaches welding temperature, and this vapor — generated at the surface and, in lap joints, at the sandwiched faying surface — must escape through the molten weld pool before it solidifies. If the vapor cannot escape fast enough, it becomes trapped as porosity. Bare steel has no equivalent vapor source, so this specific porosity mechanism does not occur.

What gap should I use when laser welding galvanized lap joints?

0.1–0.3 mm depending on material thickness and zinc coating weight — thinner material with lighter coating (Z275, approximately 20 μm) needs a smaller gap (0.05–0.15 mm); thicker material with heavier coating (Z450+) needs a larger gap (0.20–0.30 mm). The gap provides an escape channel for zinc vapor generated at the faying surface. Mechanical spacer tabs formed into one sheet at 50–100 mm intervals are the most repeatable method for production.

Should I remove the zinc coating before welding galvanized steel?

For general production fabrication, the gap technique combined with parameter optimization (slower start, wobble or pulsed power mode) usually produces acceptable weld quality without removing the coating. For critical structural welds, hermetic seals, or cosmetic applications requiring porosity-free welds, mechanical grinding or laser pre-ablation of the zinc coating in the joint area eliminates the porosity mechanism at its source, at the cost of an added process step and the need for post-weld corrosion protection at the stripped zone.


References

  1. AWS D19.0, Welding Zinc-Coated Steel, AWS, Miami, FL, current edition. (Galvanized steel welding procedures; gap technique specifications; porosity prevention methods — the primary industry standard for welding zinc-coated steel.)
  2. ASM Handbook, Volume 6: Welding, Brazing, and Soldering, 10th Edition. ASM International, 1993. (Zinc vaporization mechanism during welding; porosity formation in coated steel welding; coating weight classifications.)
  3. ASTM A653/A653M, Standard Specification for Steel Sheet, Zinc-Coated (Galvanized) or Zinc-Iron Alloy-Coated (Galvannealed) by the Hot-Dip Process, ASTM International, current edition. (Zinc coating weight classifications Z275, Z450, etc. — the coating specification referenced for the gap sizing guidance in this article.)
  4. ARCUSCNC, Laser Welding Machine Operation Manual, ARCUSCNC, 2024. (Wobble welding and pulsed power mode configuration; parameter settings for coated material — the machine-specific reference for the process adjustment recommendations in this article.)
Dr. Liu Che